Actual Certified Material Test Report
Alloy |
ER4130 |
Diameter |
3/32" |
Heat Number |
12/1609 |
Date Entered |
2/9/2005 |
Entered By |
dbf |
CHEMICAL ANALYSIS: |
|
Aluminum (Al) |
.016 |
Carbon (C) |
.310 |
Chromium (Cr) |
.920 |
Copper (Cu) |
.140 |
Manganese (Mn) |
.540 |
Molybdenum (Mo) |
.210 |
Nickel (Ni) |
.030 |
Phosphorus (P) |
.0030 |
Silicon (Si) |
.240 |
Sulfur (S) |
.0060 |
Titanium (Ti) |
.004 |
Vanadium (V) |
.004 |
Typical Certified Material Test Report
Alloy |
ER4130 |
Date Entered |
7/28/2016 |
CHEMICAL ANALYSIS: |
|
Aluminum (Al) |
.016 |
Carbon (C) |
.31 |
Chromium (Cr) |
.92 |
Copper (Cu) |
.21 |
Manganese (Mn) |
.52 |
Molybdenum (Mo) |
.20 |
Nickel (Ni) |
.05 |
Phosphorus (P) |
.005 |
Silicon (Si) |
.25 |
Sulfur (S) |
.005 |
Vanadium (V) |
.004 |
Tizr |
.004 |
CONDITION A: Tensile strength 145,000psi PWHY@1150F, Normalize 1550F and Temper @1050F Yield strength 130,000psi Elongation 11%-32RC |
|
CONDITION B: Tensile Strength 110,000psi PWHT @1150f Yield strength 90,000psi, Elongation 20%-26RC |
|
CONDITION C: Tensile Strength 178,000psi PWHT @1150F, Normalize 1650F and Temper 800F Yield strength 170,000psi, Elongation 7%-40RC |