Actual Certified Material Test Report

Alloy

ER308LSI (AWS A5.9)

Diameter

.030"

Heat Number

V3487

Date Entered

8/2/2004

Entered By

JLA

CHEMICAL ANALYSIS:

Carbon (C)

0.0220

Chromium (Cr)

20.2200

Copper (Cu)

0.2100

Manganese (Mn)

1.7200

Molybdenum (Mo)

0.0900

Nickel (Ni)

10.0500

Nitrogen (N)

0.0490

Phosphorus (P)

0.0270

Silicon (Si)

0.7800

Sulfur (S)

0.0120

Titanium (Ti)

0.0050

Ferrite Schaeffler

13.000

Ferrite Delong

11.000

Typical Certified Material Test Report

Alloy

ER308LSI (AWS A5.9)

Date Entered

9/10/2012

Entered By

BY

CHEMICAL ANALYSIS:
(Single values are maximum)

Carbon (C)

0.03

Chromium (Cr)

19.5-22.0

Copper (Cu)

0.75

Manganese (Mn)

1.0-2.5

Molybdenum (Mo)

0.75

Nickel (Ni)

9.0-11.0

Phosphorus (P)

0.03

Silicon (Si)

0.65-1.00

Sulfur (S)

0.03

YIELD STRENGTH. ksi: 55

TENSILE STRENGTH, ksi: 85

% ELONGATION min: 40

Welding Material Sales certifies that the above chemical test results are correct and conform to the AWS specification stated as contained in the records of the company. The test report represents the actual attributes of the heat number furnished.